Wood Properties | Trait | Trait definition (unit) | Mean | SD | CPV |
---|---|---|---|---|---|
Mechanical properties (M) | LGS | Mean Longitudinal Growth Strain (μm) | 72 | 13 | 0.18 |
 | Ep | Primary value of Modulus of elasticity (GPa) | 9 | 1 | 0.14 |
 | E30 | Mean Modulus of elasticity at 30 months (GPa) | 11 | 1 | 0.12 |
 | E2i | Modulus of elasticity after inflection point (GPa) | 14 | 2 | 0.13 |
Technological properties (T) | SId | Splitting Index at 1 day | 1.19 | 0.48 | 0.41 |
 | SIw | Splitting Index at 1 week | 0.96 | 0.49 | 0.51 |
 | SIm | Splitting Index at 1 months | 1.06 | 0.48 | 0.45 |
Physical properties (P) | Pil14 | Pilodyn at 14 months (mm) | 25 | 3 | 0.10 |
 | Pil26 | Pilodyn at 26 months (mm) | 26 | 2 | 0.09 |
 | Pil38 | Pilodyn 38 months (mm) | 25 | 3 | 0.11 |
 | Pil51 | Pilodyn 51 months (mm) | 28 | 2 | 0.09 |
 | Pil59 | Pilodyn 59 months (mm) | 27 | 3 | 0.11 |
 | Pil59u | Pilodyn, under bark, 59 months (mm) | 22 | 3 | 0.13 |
 | μD | Mean microdensity (g.dm-3) | 501 | 40 | 0.08 |
Chemical composition (C) | Text | Extractive content (%) | 3.70 | 0.62 | 0.17 |
 | Klass | Lignin content (wood %) | 24.6 | 0.8 | 0.03 |
 | G | G content (μmol.g-1 lignin) | 624 | 77 | 0.12 |
 | S | S content (μmol.g-1 lignin) | 2504 | 405 | 0.16 |
 | S/G | S/G ratio | 4.03 | 0.53 | 0.13 |
 | Poly | Polyphenols content (mg.g-1) | 4551 | 1742 | 0.38 |
 | Fla | Flavanols content (mg.g-1) | 249 | 148 | 0.59 |
Anatomical properties (A) | FWL | weighted fibre length (mm) | 1.28 | 0.05 | 0.04 |
 | FW | Fibre width (μm) | 33 | 1 | 0.03 |
 | Coar | Fibre coarseness (μg.mm-1) | 0.0966 | 0.0025 | 0.03 |
 | Curl | Fibre curl index (%) | 15.8 | 1.1 | 0.07 |
Growth (G) | Ht59 | Total height at 59 month old (m) | 24.2 | 2.4 | 0.10 |
 | Cir59 | Circumference (1.3 m) at 59 month old (cm) | 54 | 9 | 0.16 |